Wide Width Tensile Testing

Home / Testing Guides / Wide Width Tensile Testing

Tensile testing is among the most standard tests performed by universal testing machines yet depending on how the test specimen is used in its native environment, setting up the tensile test method is not always straightforward. Wide width tensile testing is a type of tensile testing procedure used with specimens that are prepared with wider width than the standard tensile specimen coupons. This blog posts covers wide width tensile testing, standards outlining wide width testing methods, and the necessary equipment.

Wide width tensile testing is a tensile test method that covers the measurement of tensile load elongation characteristics as well as the offset modulus, secant modulus, and breaking toughness. The main difference of this method and other methods for measuring strip tensile properties is the width of the specimen.

Why wide width tensile testing?

Materials that are often tested in wide width forms include fabrics and geotextiles including woven and nonwoven geotextiles, geocomposites, knitted geotextiles, and felts. The recommended specimen width for such materials is much wider than the width of the specimen used to run strip test methods such as ASTM D5035. When force is applied, certain fabrics have a tendency to neck down in the gauge length area. The greater specimen width minimizes the contraction effect and provides a closer relationship to the expected geotextile behavior in the field.

Geotextiles are any permeable textile material used with foundation, soil, rock, earth, or any other geotechnical engineering related material, as an integral part of a man-made project, structure, or system.

ASTM D4595 Test Method for Tensile Properties of Geotextiles by the Wide-Width Strip Method

ASTM D4595 is a method covering the wide width tensile testing of geotextile specimen. Each wide width specimen is gripped across its entire width in grip jaws and pulled in tension with a constant rate of extension type tensile testing machine.Force is applied until specimen ruptures and tensile properties such as tensile strength, elongation, initial and secant modulus, and breaking toughness are calculated.

The specimen size per ASTM D4595 is 8 by 8 inches and the recommended grip jaw size is 8 by 2 inches. Wet and dry specimens may be tested following this method. Refer to the ASTM standard for further details.

ISO 10319 Geosynthetics — Wide-width tensile test

Similar to ASTM D4595, ISO 10319 outlines a standardized procedure to pull wide width geosynthetic specimens in tension until rupture. This standard, however, specifies different dimensions based on the material type: nonwoven geotextiles, woven geotextiles, geogrids with one axis (shown below), geogrids with two and four axes, geogrids with three axes, and metallic geotextiles. Tensile properties measured include the tensile strength and strain data and secant stiffness.

Diagram of a geogrid
Figure 1 – Typical geogrid with one axis (from ISO 10319)

Other standards that can be followed include ASTM D6637 Test Method for Determining Tensile Properties of Geogrids by the Single or Multi-Rib Tensile Method and ISO 10321 Geosynthetics — Tensile test for joints/seams by wide-width strip method.

Recommended Equipment

As specified in the testing standards, a constant rate of extension type tensile testing machine is recommended for testing wide width specimen. All ADMET systems are servo controlled and meet the standardized requirements.

The eXpert 7600 single column testing machines can be used for lower force applications while the eXpert 2600 series dual column electromechanical testing systems have a broader range of force capacity, from 0.22kN (50lbf) to 400kN (90,000lbf). In addition, eXpert 1600 series servo-hydraulic frames offer capacities up to 600kN (135,000lbf).

Universal testing machines must be equipped with grips that have grip jaws covering the whole width of the specimen.

Standard grip options that accommodate wide widths include pneumatic grips, wedge grips, hydraulic grips, and self-tightening grips such as scissor grips.

If specimen ruptures on the edge of the grip jaws, we recommend using capstan or roller grips. Samples must be able to fold and be placed in the roller drum without causing damage to the material structure.

Chart of grip specifications for wide samples

For geotextiles made from glass fibers, custom grips may be required to avoid slippage or damage from jaws.

Use a universal joint to allow the grip to rotate in the plane of the fabric to ensure vertical alignment in the direction of test.

When information on strain is required, consider utilizing an axial extensometer to measure strain data.

Conclusion

If you’re interested in learning more about wide width tensile testing equipment, please reach out to one of our Sales Engineers. We may ask for specimens to be sent to the ADMET lab to ensure the right equipment is recommended for you to achieve your testing goals.

By: Deniz Yalcin | Published on: May 16, 2019 | Last Updated: January 6, 2026

Just Ask!

Need Help With Your Wide Width Tensile Testing?

Our engineers are ready to help you!

spiral arrow graphic

Testing Guides

  • Medical Adhesive Testing Basics

    Medical adhesives are specialized substances used to bond medical devices, tissues, or other components together. They must comply with strict biocompatibility requirements and are vital in surgeries, wound care, and medical equipment manufacturing.
  • Deflection & How To Use A Deflectometer

    Deflection, in materials science, is the amount a material deflects under compressive load. It is a displacement measurement with units expressed in millimeters or inches. This post goes over frequently asked questions around deflection measurements and equipment used to measure them.
  • Peel Strength Testing

    Peel strength is calculated by averaging the load to peel the specimen and dividing it by unit width of the bond line.
  • Tensile Testing FAQs

    Tensile testing FAQs including How does the loading rate affect tensile properties? How does grip-specimen engagement affect tensile properties? What is the best way to measure small strains? are answered.