Summary of Test
ASTM F564 details three types of tests commonly conducted during the product development process of metallic staples to be used in medical applications related to bone.
This post is intended to help you understand the basic procedures and the equipment needed to complete the fatigue, pull-out strength, fixation strength, and bending tests explained in the specification. For complete instructions, please refer to ASTM F564.
Recommended Equipment
Testing Procedure
Test 1 – Bending Fatigue Tests of Metallic Bone Staples
- Fix and align each staple leg into the extension block using the specified filling agent.
- Place the staple and extensions into a 4-point-bend fixture.
- Begin to apply cyclic loads to create a non-permanent bend in the staple.
- Continue test until specimen failure.
- Place another staple and extensions into an axial (tension/compression) fixture.
- Begin to apply cyclic loads to create a non-permanent bend in the staple.
- Continue test until specimen failure.
Test 2 – Pull-Out Fixation Strength of Metallic Bone Staples
- Fix a thin and flat metal or fabric strap onto a piece of bone or bone substitute using a staple. Make sure to insert the staple following the correct surgical/manufacturer indicated processes. The staple should not penetrate the strap but rather act as a loop to hold the bone sample to the strap.
- Fix the bone sample into one bottom machine grip. Connect the ends of the strap and fix them into the other machine grip.
- Begin to the sample at a constant rate.
- Stop the test at visible tearing or rupture of the strap, fracture of the bone, or loosening of the staple.

Test 3 – Soft Tissue Fixation Strength of Metallic Bone Staples
- Secure a piece of soft tissue or tissue substitute onto a piece of bone or bone substitute using one or multiple staples. Make sure to insert the staple following the correct surgical/manufacturer indicated processes.
- Fix the bone sample into one bottom machine grip. Secure the tissue sample on the other machine grip.
- Begin pulling the sample at a constant rate.
- Stop the test at visible tearing or rupture of the strap, fracture of the bone, or loosening of the staple.
Test 4 – Static Bending of Metallic Bone Staples
- Before testing the staple, measure the deflection under testing load of the bend fixtures and gripping devices as described in the specification. You might have to adjust your results depending on how much these devices bend.
- Fix and align each staple leg into the extension block using the specified filling agent.
- Place the extension blocks onto the bottom of the 4-point-bend-fixture.
- Apply downward force onto the extension blocks with the top of the 4-point-bend fixture at the constant rate specified.
- Continuously graph load versus displacement.
- Continue the test until enough data is gathered to accurately assess the stiffness of the sample.

Just Ask!