Summary of Test
Penetration resistance is a vital part of the quality of thin, flexible materials in which any sharp-edged item pointed downward will not break past the barrier of a film or laminate. ASTM F1306 is a specification regarding the slow rate penetration resistance properties of flexible barrier films and laminates. Thin, flexible specimens must be of uniform thickness at 0.0025 mm or 0.0001 in.
A universal testing machine with a recording device and penetration probe are needed to perform this test. Ultimately, the force, energy, and elongation to perforation of the material are observed. Before conducting ASTM F1306, one should read the whole ASTM specification.
Recommended Equipment
Testing Procedure
- Cut each test material into at least 5 samples of 3 in x 3 in square and clamp one at a time in test fixture.
- Clamp the specimen in the holder and lower the crosshead probe as close to the film specimen without making contact.
- Continue the test at a constant rate of crosshead movement according to the specification and continue until the sample ruptures. Return the crosshead to the home position after rupture.
Just Ask!
Questions about running ASTM F1306 on your system?